S275N
2023-05-17 16:02:38
來源:鋼鐵之家
閱讀量:0
牌號
S275N
歐標(biāo)鋼號
1.0490
對應(yīng)標(biāo)準(zhǔn)
EN 10025-3-2004
熱軋結(jié)構(gòu)鋼鋼材 第3部分:正火/正火軋制可焊接的細(xì)晶結(jié)構(gòu)鋼 Hot rolled products of structural steels - Part 3: Technical delivery conditions for normalized/normalized rolled weldable fine grain structural steels
歸類
碳鋼
S275N 化學(xué)元素成分含量(%)
成分
C
Si
Mn
P ①
S ①②
Cr
Ni
Cu ④
Mo
N
Ti
V
Nb
Al ③
最小值
-
-
0.5
-
-
-
-
-
-
-
-
-
-
0.02
最大值
0.18
0.4
1.5
0.03
0.025
0.3
0.3
0.55
0.1
0.015
0.05
0.05
0.05
-
① For long products the P and S content can be 0.005% higher.
② For railway applications a maximum S content of 0.010% may be agreed at the time of enquiry and order.
③ If sufficient other N-binding elements are present the minimum total Al content does not apply.
④ Cu content above 0.40% may cause hot shortness during hot forming.
S275N 機(jī)械性能
公稱厚度
t
mm
抗拉強(qiáng)度 σb
Mpa
屈服點(diǎn) σs
Mpa
斷后伸長率或延伸率 δ
%
t≤16
370~510
≥275
≥24
16
370~510
≥265
≥24
40
370~510
≥255
≥24
63
370~510
≥245
≥23
80
370~510
≥235
≥23
100
350~480
≥225
≥23
150
350~480
≥215
≥23
200
350~480
≥205
≥23
For plate,strip and wide flats with widths≥600mm the direction transverse (t) to the rolling direction applies. For all other products the values apply for the direction parallel (l) to the rolling direction
①在此測試溫度下的最小沖擊吸收能量
1 近似對照表 優(yōu)質(zhì)碳素結(jié)構(gòu)鋼
日本
美國
德國
歐標(biāo)
英國
JIS
ASTM
DIN EN/DIN
W-Nr.
EN
數(shù)字牌號
BS EN/BS
SM400B
A572Gr.42
A633A
StE285
1.0486
S275N
FeE275KGN①
1.0490
43DD
注:本資料來源于互聯(lián)網(wǎng)的公開資源整理,我們不保證這些資料的準(zhǔn)確性、完整性和適用性。這些資料僅供您參考,不應(yīng)用于任何商業(yè)用途或決策依據(jù)。本資料所記載的技術(shù)信息是說明產(chǎn)品的代表性特點(diǎn)和性能的參考值,對于因誤用或不當(dāng)使用本資料所記載的信息等而造成的損害恕難承擔(dān)責(zé)任,敬請周知。